Corrosion Resistant
Hyperion Code: N and C Grades
Dimension: n/a
Description: Standard tungsten carbide ready-to-press powder grades designed for superior corrosion resistance.
Standard Corrosion Resistant Grades
Hyperion Carbide Grades |
Chemical Composion (weight %) |
Sintering Temperature (°C) |
Density (g/cm3) | Hardness | Sintered Grain Size (μm) | |||||||
WC | Co | Ni | Cr3C2 | TiC | TaC + NbC | Other Elements | Vickers (HV30) | Rockwell (HRA) | ||||
N6 | 93.85 | - | 6 | 0.15 | - | - | - | 1450 | 14.95 | 1500 | 91.4 | 1.0 |
N10 | 89.5 | - | 10 | 0.50 | - | - | - | 1410 | 14.41 | 1350 | 89.8 | 1.0 |
C2 | 93.1 | 0.5 | 6 | - | - | - | 0.4 | 1450 | 14.90 | 1390 | 90.3 | 3.0 |
C4 | 84 | - | 5.65 | - | 8.75 | - | 1.6 | 1450 | 12.65 | 1750 | 93.1 | 1.5 |
Further information
All data shown are typical values.
Your Hyperion salesperson can offer their expertise in selecting either the standard ready-to-press powder or a tailor-made powder best suited to solve your needs.